Metals
|
Longitudinal Velocity
|
Shear
Velocity
|
Surface Velocity
|
Density
g/cm3
|
Acoustic Impedance
g/cm2-secx105
|
|
cm/ms
|
in/ms
|
cm/ms
|
in/ms
|
cm/ms
|
in/ms
|
|
Aluminum
|
.632
|
.2488
|
.313
|
.1232
|
N/A
|
N/A
|
2.70
|
17.10
|
|
AL 1100-0 (2SO)
|
.635
|
.25
|
.310
|
.122
|
.290
|
.114
|
2.71
|
17.20
|
|
AL 2014 (14S)
|
.632
|
.2488
|
.307
|
.1209
|
N/A
|
N/A
|
2.80
|
17.80
|
|
AL 2024 T4 (24ST)
|
.637
|
.2508
|
.316
|
.1244
|
.295
|
.116
|
2.77
|
17.60
|
|
AL 2117 T4 (17ST)
|
.650
|
.2559
|
.312
|
.1228
|
N/A
|
N/A
|
2.80
|
18.20
|
|
|
|
|
|
|
|
|
|
|
|
Bearing Babbit
|
.230
|
.0906
|
N/A
|
N/A
|
N/A
|
N/A
|
1.10
|
23.20
|
|
Beryllium
|
1.29
|
.5079
|
.888
|
.3496
|
.787
|
.310
|
1.82
|
23.50
|
|
Bismuth
|
.218
|
.0858
|
.110
|
.0433
|
N/A
|
N/A
|
9.80
|
21.40
|
|
Brass
|
.428
|
.1685
|
.230
|
.0906
|
N/A
|
N/A
|
8.56
|
36.70
|
|
Brass,
Half Hard
|
.383
|
.1508
|
.205
|
.0807
|
N/A
|
N/A
|
8.10
|
31.02
|
|
Brass, Naval
|
.443
|
.1744
|
.212
|
.0835
|
.195
|
.0770
|
8.42
|
37.3
|
|
Bronze, Phospho
|
.353
|
.139
|
.223
|
.0878
|
.201
|
.0790
|
8.86
|
31.28
|
|
|
|
|
|
|
|
|
|
|
Cadmium
|
.278
|
.1094
|
.150
|
.0591
|
N/A
|
N/A
|
8.64
|
24.02
|
|
Cesium
(28.5°
C)
|
.0967
|
.0381
|
N/A
|
N/A
|
N/A
|
N/A
|
1.88
|
1.82
|
|
Columbium
|
.492
|
.1937
|
.210
|
.0827
|
N/A
|
N/A
|
8.57
|
42.16
|
|
Constantan
|
.524
|
.2063
|
.104
|
.0409
|
N/A
|
N/A
|
8.88
|
46.53
|
|
Copper
|
.466
|
.1835
|
.0890
|
.035
|
.193
|
.0760
|
8.93
|
41.61
|
|
|
|
|
|
|
|
|
|
|
|
Gallium
|
.274
|
.1079
|
N/A
|
N/A
|
N/A
|
N/A
|
5.95
|
16.3
|
|
Germanium
|
.541
|
.213
|
N/A
|
N/A
|
N/A
|
N/A
|
5.47
|
29.59
|
|
Gold
|
.324
|
.1276
|
.120
|
.0472
|
N/A
|
N/A
|
19.32
|
62.6
|
|
Hafnium
|
.384
|
.1512
|
N/A
|
N/A
|
N/A
|
N/A
|
N/A
|
N/A
|
|
Inconel
|
.572
|
.2252
|
N/A
|
N/A
|
.279
|
.110
|
8.25
|
47.19
|
|
Indium
(156°
C)
|
.222
|
.0874
|
N/A
|
N/A
|
N/A
|
N/A
|
7.30
|
16.21
|
|
Iron
|
.590
|
.2323
|
.323
|
.1272
|
.279
|
.110
|
7.70
|
45.43
|
|
Iron, Cast
|
.480
|
.189
|
.240
|
.0945
|
N/A
|
N/A
|
7.80
|
37.44
|
|
|
|
|
|
|
|
|
|
|
Lead
|
.216
|
.085
|
.070
|
.0276
|
.0630
|
.0248
|
11.4
|
24.62
|
|
Lead, 5% Antinomy
|
.217
|
.0854
|
.081
|
.0319
|
.0740
|
.0291
|
1.9
|
23.65
|
|
Magnesium
|
.631
|
.2484
|
N/A
|
N/A
|
N/A
|
N/A
|
1.74
|
10.98
|
|
Magnesium
(AM-35)
|
.579
|
.228
|
.310
|
.122
|
.287
|
.113
|
1.74
|
10.07
|
|
Magnesium
(FS-1)
|
.547
|
.2154
|
.303
|
.1193
|
N/A
|
N/A
|
1.69
|
9.24
|
|
Magnesium
(J-1)
|
.567
|
.2232
|
.301
|
.1185
|
N/A
|
N/A
|
1.70
|
9.64
|
|
Magnesium
(M)
|
.576
|
.2268
|
.309
|
.1217
|
N/A
|
N/A
|
1.75
|
10.08
|
|
Magnesium
(O-1)
|
.580
|
.2283
|
.304
|
.1197
|
N/A
|
N/A
|
1.82
|
10.56
|
|
Magnesium
(ZK-60A-TS)
|
.571
|
.2248
|
.305
|
.1201
|
N/A
|
N/A
|
1.83
|
10.45
|
|
Manganese
|
.466
|
.1835
|
.235
|
.0925
|
N/A
|
N/A
|
7.39
|
34.44
|
|
Molybdenum
|
.629
|
.2476
|
.335
|
.1319
|
.311
|
.122
|
10.2
|
64.16
|
|
Monel
|
.602
|
.237
|
.272
|
.1071
|
.196
|
.0772
|
8.83
|
53.16
|
|
|
|
|
|
|
|
|
|
|
|
Nickel
|
.563
|
.2217
|
.296
|
.1165
|
.264
|
.104
|
8.88
|
49.99
|
|
Platinum
|
.396
|
.1559
|
.167
|
N/A
|
N/A
|
N/A
|
21.4
|
84.74
|
|
Plutonium
|
.179
|
.0705
|
N/A
|
N/A
|
N/A
|
N/A
|
N/A
|
28.2
|
|
Plutonium
(1% Gallium)
|
.182
|
.0717
|
N/A
|
N/A
|
N/A
|
N/A
|
N/A
|
28.6
|
|
Potassium
(100°
C)
|
.182
|
.0717
|
N/A
|
N/A
|
N/A
|
N/A
|
.83
|
1.51
|
|
Radium
|
.0822
|
.0324
|
.111
|
.0437
|
.103
|
.0404
|
5.0
|
4.11
|
|
|
|
|
Rubidium
|
.126
|
.0496
|
N/A
|
N/A
|
N/A
|
N/A
|
1.53
|
1.93
|
|
Silver
|
.360
|
.1417
|
.159
|
.0626
|
N/A
|
N/A
|
1.5
|
37.8
|
|
Silver, Nickel
|
.462
|
.1819
|
.232
|
.0913
|
.169
|
.0665
|
8.75
|
40.43
|
|
Silver, German
|
.476
|
.1874
|
N/A
|
N/A
|
N/A
|
N/A
|
8.70
|
41.41
|
|
Steel, 302 Cres
|
.566
|
.2228
|
.312
|
.1228
|
.312
|
.123
|
8.03
|
45.45
|
|
Steel, 347 Cres
|
.574
|
.226
|
.309
|
.1217
|
N/A
|
N/A
|
7.91
|
45.4
|
|
Steel, 410 Cres
|
.739
|
.2909
|
.299
|
.1177
|
.216
|
.0850
|
7.67
|
56.68
|
|
Steel, 1020
|
.589
|
.2319
|
.324
|
.1276
|
N/A
|
N/A
|
7.71
|
45.41
|
|
Steel, 1095
|
.590
|
.2323
|
.319
|
.1256
|
N/A
|
N/A
|
7.80
|
46.02
|
|
Steel, 4150, Rc14
|
.586
|
.2307
|
.279
|
.1098
|
N/A
|
N/A
|
7.84
|
45.94
|
|
Steel, 4150, Rc18
|
.589
|
.2319
|
.318
|
.1252
|
N/A
|
N/A
|
7.82
|
46.06
|
|
Steel, 4150, Rc43
|
.587
|
.2311
|
.320
|
.126
|
N/A
|
N/A
|
7.81
|
45.84
|
|
Steel, 4150, Rc64
|
.582
|
.2291
|
.277
|
.1091
|
N/A
|
N/A
|
7.80
|
45.4
|
|
|
|
|
|
|
|
|
|
|
|
Steel, 4340
|
.585
|
.2303
|
.128
|
.0504
|
N/A
|
N/A
|
7.80
|
45.63
|
|
Tantalum
|
.410
|
.1614
|
.114
|
.0449
|
N/A
|
N/A
|
16.6
|
68.06
|
|
Thallium
(302°
C)
|
.162
|
.0638
|
N/A
|
N/A
|
N/A
|
N/A
|
11.9
|
19.28
|
|
Thorium
|
.240
|
.0945
|
.156
|
.0614
|
N/A
|
N/A
|
11.3
|
27.12
|
|
Tin
|
.332
|
.1307
|
.167
|
.0657
|
N/A
|
N/A
|
7.29
|
24.2
|
|
Titanium
|
.607
|
.239
|
.331
|
.1303
|
N/A
|
N/A
|
4.50
|
27.32
|
|
|
|
|
|
|
|
|
|
|
|
Titanium Carbide
|
.827
|
.3256
|
.516
|
.2031
|
N/A
|
N/A
|
5.15
|
42.59
|
|
Tungsten
|
.518
|
.2039
|
.287
|
.113
|
.265
|
.104
|
19.25
|
99.72
|
|
Uranium
|
.338
|
.1331
|
.196
|
.0772
|
N/A
|
N/A
|
18.9
|
63.88
|
|
Uranium Dioxide
|
.518
|
.2039
|
N/A
|
N/A
|
N/A
|
N/A
|
6.03
|
31.24
|
|
Vanadium
|
.600
|
.2362
|
.278
|
.1094
|
N/A
|
N/A
|
6.03
|
36.18
|
|
Zinc
|
.417
|
.1642
|
.0949
|
.0374
|
N/A
|
N/A
|
7.10
|
29.61
|
|
Zircaloy
|
.472
|
.1858
|
.093
|
.0366
|
N/A
|
N/A
|
9.03
|
42.6
|
|
Zirconium
|
.465
|
.1831
|
.0886
|
.0349
|
N/A
|
N/A
|
6.48
|
30.1
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
-
|
|
|