| Aluminum |
|
|
|
|
|
|
| Pure |
61.00
|
3.538E+07
|
2.826E-08
|
ECTM
|
|
|
| 99.99% |
64.94
|
3.767E+07
|
2.655E-08
|
CSNDT
|
|
|
| 99.99% |
64.94
|
3.767E+07
|
2.655E-08
|
ALASM
|
|
|
| Red
X-8 Cond. Stress Relieved |
29.00
|
1.682E+07
|
5.945E-08
|
CSNDT
|
|
|
| Red
X-8 As Cast |
26.00
|
1.508E+07
|
6.631E-08
|
CSNDT
|
|
|
| 11S
Cond. T3 |
40.00
|
2.320E+07
|
4.310E-08
|
CSNDT
|
|
|
| 13 |
39.00
|
2.262E+07
|
4.421E-08
|
CSNDT
|
|
|
| 14S
Cond. "0" |
50.00
|
2.900E+07
|
3.448E-08
|
CSNDT
|
|
|
| 14S
Cond. T6 |
40.00
|
2.320E+07
|
4.310E-08
|
CSNDT
|
|
|
| 17S
Cond. "0" |
45.00
|
2.610E+07
|
3.831E-08
|
CSNDT
|
|
|
| 17S
Cond. T4 |
30.00
|
1.740E+07
|
5.747E-08
|
CSNDT
|
|
|
| 18S
Cond. "0" |
50.00
|
2.900E+07
|
3.448E-08
|
CSNDT
|
|
|
| 18S
Cond. T61 |
40.00
|
2.320E+07
|
4.310E-08
|
CSNDT
|
|
|
| 2S
Cond. "0" |
59.00
|
3.422E+07
|
2.922E-08
|
CSNDT
|
|
|
| 2S
Cond. H18 |
57.00
|
3.306E+07
|
3.025E-08
|
CSNDT
|
|
|
| 24S
Cond. "0" |
50.00
|
2.900E+07
|
3.448E-08
|
CSNDT
|
|
|
| 24S
Cond. T4 |
30.00
|
1.740E+07
|
5.747E-08
|
CSNDT
|
|
|
| 24S
Cond. T6 |
40.00
|
2.320E+07
|
4.310E-08
|
CSNDT
|
|
|
| 3S
Cond. "0" |
50.00
|
2.900E+07
|
3.448E-08
|
CSNDT
|
|
|
| 3S
Cond. H 12 |
42.00
|
2.436E+07
|
4.105E-08
|
CSNDT
|
|
|
| 3S
Cond. H 14 |
41.00
|
2.378E+07
|
4.205E-08
|
CSNDT
|
|
|
| 3S
Cond. H 18 |
40.00
|
2.320E+07
|
4.310E-08
|
CSNDT
|
|
|
| 32S
Cond. "0" |
40.00
|
2.320E+07
|
4.310E-08
|
CSNDT
|
|
|
| 32S
Cond. T6 |
35.00
|
2.030E+07
|
4.926E-08
|
CSNDT
|
|
|
| 40E |
35.00
|
2.030E+07
|
4.926E-08
|
CSNDT
|
|
|
| 43
(Annealed) |
42.00
|
2.436E+07
|
4.105E-08
|
CSNDT
|
|
|
| 43
As Cast |
37.00
|
2.146E+07
|
4.660E-08
|
CSNDT
|
|
|
| A51S
Cond. "0" |
55.00
|
3.190E+07
|
3.135E-08
|
CSNDT
|
|
|
| A51S
Cond. T4 and T6 |
45.00
|
2.610E+07
|
3.831E-08
|
CSNDT
|
|
|
| 52S
Cond. "0" and H 38 |
35.00
|
2.030E+07
|
4.926E-08
|
CSNDT
|
|
|
| 53S
Cond. "0" |
45.00
|
2.610E+07
|
3.831E-08
|
CSNDT
|
|
|
| 53S
Cond. T4 and T6 |
40.00
|
2.320E+07
|
4.310E-08
|
CSNDT
|
|
|
| 56S
Cond. "0" |
29.00
|
1.682E+07
|
5.945E-08
|
CSNDT
|
|
|
| 56S
Cond. H 38 |
27.00
|
1.566E+07
|
6.386E-08
|
CSNDT
|
|
|
| 61S
Cond. "0" |
45.00
|
2.610E+07
|
3.831E-08
|
CSNDT
|
|
|
| 61S
Cond. T4 and T6 |
40.00
|
2.320E+07
|
4.310E-08
|
CSNDT
|
|
|
| 75S
Cond. T6 |
30.00
|
1.740E+07
|
5.747E-08
|
CSNDT
|
|
|
| 85 |
28.00
|
1.624E+07
|
6.158E-08
|
CSNDT
|
|
|
| |
|
|
|
|
|
|
| Aluminum
Allcast |
|
|
|
|
|
|
| As
Cast |
27.00
|
1.566E+07
|
6.386E-08
|
CSNDT
|
|
|
| Cond.
Sol. H.T. & Stress Relieved |
36.00
|
2.088E+07
|
4.789E-08
|
CSNDT
|
|
|
| Sol
H.T. and Aged |
30.00
|
1.740E+07
|
5.747E-08
|
CSNDT
|
|
|
| Stress
Relieved |
30.00
|
1.740E+07
|
5.747E-08
|
CSNDT
|
|
|
| |
|
|
|
|
|
|
| Aluminum
Alloy (Wrought) |
|
|
|
|
|
|
| 1050-0 |
61.30
|
|
2.810E-08
|
ALASM
|
|
|
| 1060-O |
62.00
|
|
2.780E-08
|
ALASM
|
|
|
| 1060-H18 |
61.00
|
|
2.780E-08
|
ALASM
|
|
|
| 1100 |
57.00 - 61.80
|
3.445E+07
|
2.903E-08
|
NDT Mag
|
|
|
| 1100-O |
59.00
|
|
2.920E-08
|
ALASM
|
|
|
| 1100-H18 |
57.00
|
|
3.020E-08
|
ALASM
|
|
|
| 1145-O |
61.00
|
|
2.830E-08
|
ALASM
|
|
|
| 1145-H18 |
60.00
|
|
2.830E-08
|
ALASM
|
|
|
| 1199-O |
64.50
|
|
2.670E-08
|
ALASM
|
|
|
| 1350-O |
61.80
|
|
2.790E-08
|
ALASM
|
|
|
| 1350-Hx |
61.00
|
|
2.820E-08
|
ALASM
|
|
|
| 2011-T3 |
36.00 - 36.50
|
2.103E+07
|
4.756E-08
|
NDT Mag
|
|
|
| 2011-T3
and T4 |
39.00
|
|
4.400E-08
|
ALASM
|
|
|
| 2011-T8 |
45.00
|
|
3.800E-08
|
ALASM
|
|
|
| 2014-F
and -0 |
48.60 - 50.70
|
2.880E+07
|
3.473E-08
|
NDT Mag
|
|
|
| 2014-O |
50.00
|
|
3.400E-08
|
ALASM
|
|
|
| 2014-T3
and -T4 |
32.50 - 34.80
|
1.952E+07
|
5.124E-08
|
NDT Mag
|
|
|
| 2014-T3,
T4, and T451 |
34.00
|
|
5.100E-08
|
ALASM
|
|
|
| 2014-T6 |
38.00 - 39.70
|
2.253E+07
|
4.438E-08
|
NDT Mag
|
|
|
| 2014-T6,
T651, and T652 |
40.00
|
|
4.300E-08
|
ALASM
|
|
|
| 2017-F |
49.30 - 49.50
|
2.865E+07
|
3.490E-08
|
NDT Mag
|
|
|
| 2017-O |
50.00
|
|
3.500E-08
|
ALASM
|
|
|
| 2017-T4 |
34.00
|
|
5.000E-08
|
ALASM
|
|
|
| 2024-F |
46.80 - 48.50
|
2.764E+07
|
3.618E-08
|
NDT Mag
|
|
|
| 2024-O |
50.00
|
|
3.400E-08
|
ALASM
|
|
|
| 2024-T3 |
28.60 - 36.10
|
1.876E+07
|
5.330E-08
|
NDT Mag
|
|
|
| 2024-T36 |
29.10 - 29.50
|
1.699E+07
|
5.884E-08
|
NDT Mag
|
|
|
| 2024-T3,
T36, T351, T361, and T4 |
30.00
|
|
5.700E-08
|
ALASM
|
|
|
| 2024-T4 |
28.80 - 31.00
|
1.734E+07
|
5.766E-08
|
NDT Mag
|
|
|
| 2024-T6,
T81, T851, and T861 |
38.00
|
|
4.500E-08
|
ALASM
|
|
|
| 2036-O |
52.00
|
|
3.320E-08
|
ALASM
|
|
|
| 2036-T4 |
41.00
|
|
4.210E-08
|
ALASM
|
|
|
| 2048-T851 |
42.00
|
|
4.000E-08
|
ALASM
|
|
|
| 2124-O |
50.00
|
|
3.450E-08
|
ALASM
|
|
|
| 2124-T851 |
39.00
|
|
4.421E-08
|
ALASM
|
resistivity
converted from conductivity |
|
| 2127-T4 |
42.10 - 42.40
|
2.451E+07
|
4.081E-08
|
NDT Mag
|
|
|
| 2218-T61 |
37.40
|
2.169E+07
|
4.610E-08
|
NDT Mag
|
|
|
| 2218-T61 |
38.00
|
|
4.500E-08
|
ALASM
|
|
|
| 2218-T72 |
40.00
|
|
4.300E-08
|
ALASM
|
|
|
| 2219-O |
44.00
|
|
3.900E-08
|
ALASM
|
|
|
| 2219-T31,
T37, and T351 |
28.00
|
|
6.200E-08
|
ALASM
|
|
|
| 2219-T62,
T81, T87, and T851 |
30.00
|
|
5.700E-08
|
ALASM
|
|
|
| 2319-O |
44.00
|
|
3.900E-08
|
ALASM
|
|
|
| 2618 |
40.20
|
2.332E+07
|
4.289E-08
|
NDT Mag
|
|
|
| 2618-T61 |
37.00
|
|
4.700E-08
|
ALASM
|
|
|
| 3003-O |
44.70 - 49.80
|
2.741E+07
|
3.649E-08
|
NDT Mag
|
|
|
| 3003-O |
50.00
|
|
3.400E-08
|
ALASM
|
|
|
| 3003-H14
and -H12 |
37.80 - 51.50
|
2.590E+07
|
3.861E-08
|
NDT Mag
|
|
|
| 3003-H12 |
42.00
|
|
4.100E-08
|
ALASM
|
|
|
| 3003-H14 |
41.00
|
|
4.200E-08
|
ALASM
|
|
|
| 3003-H18 |
40.00
|
|
4.300E-08
|
ALASM
|
|
|
| 3003-H24
and -H28 |
37.80 - 47.50
|
2.474E+07
|
4.043E-08
|
NDT Mag
|
|
|
| 3004 |
39.40 - 43.50
|
2.404E+07
|
4.160E-08
|
NDT Mag
|
|
|
| 3004-O |
42.00
|
|
4.100E-08
|
ALASM
|
|
|
| X3005-O |
50.10 - 50.30
|
2.912E+07
|
3.435E-08
|
NDT Mag
|
|
|
| 3105-O |
45.00
|
|
3.830E-08
|
ALASM
|
|
|
| 4032-O |
40.00
|
|
4.310E-08
|
ALASM
|
|
|
| 4032-T6 |
35.30 - 36.30
|
2.076E+07
|
4.816E-08
|
NDT Mag
|
|
|
| 4032-T6 |
36.00
|
|
4.790E-08
|
ALASM
|
|
|
| 4043-F |
52.30 - 54.30
|
3.091E+07
|
3.235E-08
|
NDT Mag
|
|
|
| 4043-O |
42.00
|
|
4.100E-08
|
ALASM
|
|
|
| 5005 |
52.30 - 52.80
|
3.048E+07
|
3.281E-08
|
NDT Mag
|
|
|
| 5005-O
and H38 |
52.00
|
|
3.320E-08
|
ALASM
|
|
|
| 5050 |
48.30 - 49.80
|
2.845E+07
|
3.515E-08
|
NDT Mag
|
|
|
| 5050-O
and H38 |
50.00
|
|
3.400E-08
|
ALASM
|
|
|
| 5052 |
33.60 - 37.60
|
2.065E+07
|
4.843E-08
|
NDT Mag
|
|
|
| 5052-O
and H38 |
35.00
|
|
4.930E-08
|
ALASM
|
|
|
| 5056 |
28.10 - 29.80
|
1.679E+07
|
5.956E-08
|
NDT Mag
|
|
|
| 5056-O |
29.00
|
|
5.900E-08
|
ALASM
|
|
|
| 5056-H38 |
27.00
|
|
6.400E-08
|
ALASM
|
|
|
| 5083 |
29.00
|
|
5.950E-08
|
ALASM
|
|
|
| 5086 |
31.00
|
|
5.600E-08
|
ALASM
|
|
|
| 5154 |
30.50 - 32.80
|
1.836E+07
|
5.448E-08
|
NDT Mag
|
|
|
|
|