| Material |
Conductivity
|
Resistivity
|
Reference
|
Notes |
|
(% IACS)
|
(Siemens/m)
|
(Ohm-m)
|
(See Below)
|
|
| Copper
and Alloys by Copper Alloy Number
|
|
|
|
|
|
| Pure (annealed) |
100.00
|
5.800E+07
|
1.724E-08
|
ECTM
|
|
| C10100, C10200 |
101.00
|
|
1.710E-08
|
MHASM2
|
|
| C10300-O61 |
99.00
|
|
1.740E-08
|
MHASM2
|
|
| C10400, C10500, C10700 (O61 temper) |
100.00
|
|
1.720E-08
|
MHASM2
|
|
| C10800-O61 |
92.00
|
|
1.870E-08
|
MHASM2
|
|
| C11000-O60 |
100-101.5
|
|
1.700E-8--1.724E-8
|
MHASM2
|
|
| C11000-H14 |
97.00
|
|
1.780E-08
|
MHASM2
|
|
| C11100 |
100.00
|
|
1.720E-08
|
MHASM2
|
|
| C11300, C11400, C11500, C11600 |
100.00
|
|
1.720E-08
|
MHASM2
|
|
| C12500, C12700, C12800, C12900, C13000 (annealed) |
98.00
|
|
1.760E-08
|
MHASM2
|
|
| C14300 |
96.00
|
|
1.800E-08
|
MHASM2
|
|
| C14310 |
85.00
|
|
2.030E-08
|
MHASM2
|
|
| C14500 |
93.00
|
|
1.860E-08
|
MHASM2
|
|
| C14700-O61 |
95.00
|
|
1.810E-08
|
MHASM2
|
|
| C15000 |
93.00
|
|
1.860E-08
|
MHASM2
|
|
| C15100 (annealed) |
95.00
|
|
1.810E-08
|
MHASM2
|
|
| C15100 (rolled) |
90.00
|
|
1.920E-08
|
MHASM2
|
|
| C15500 (annealed) |
91.00
|
|
1.900E-08
|
MHASM2
|
|
| C15710 |
90.00
|
|
1.920E-08
|
MHASM2
|
|
| C15720 |
89.00
|
|
1.940E-08
|
MHASM2
|
|
| C16200 |
90.00
|
|
1.920E-08
|
MHASM2
|
|
| C17000-TB00 (strip) |
28-33
|
|
5.2E-8--6.2E-8
|
MHASM2
|
resistivity
converted from conductivity |
| C17000-TB00 (rod, bar, plate tubing, forgings) |
17-19
|
|
9.1E-8--1.0E-7
|
MHASM2
|
resistivity
converted from conductivity |
| C17000-TB00 (billet) |
13-18
|
|
9.6E-8--1.3E-7
|
MHASM2
|
resistivity
converted from conductivity |
| C17000-TD01 (strip) |
29-34
|
|
5.0E-8--5.9E-8
|
MHASM2
|
resistivity
converted from conductivity |
| C17000-TD02 (strip) |
32-38
|
|
4.5E-8--5.4E-8
|
MHASM2
|
resistivity
converted from conductivity |
| C17000-TD04 (strip) |
35-39
|
|
4.4E-8--4.9E-8
|
MHASM2
|
resistivity
converted from conductivity |
| C17000-TD04 (rod, bar, plate tubing) |
15-17
|
|
1.0E-7--1.1E-7
|
MHASM2
|
resistivity
converted from conductivity |
| C17000-TF00 (strip) |
35-39
|
|
4.8E-8--4.8E-8
|
MHASM2
|
resistivity
converted from conductivity |
| C17000-TF00 (rod, bar, plate tubing, forgings) |
22-25
|
|
6.9E-8--7.8E-8
|
MHASM2
|
resistivity
converted from conductivity |
| C17000-TF00 (billet) |
18-25
|
|
6.9E-8--9.6E-8
|
MHASM2
|
resistivity
converted from conductivity |
| C17000-TH01 (strip) |
36-41
|
|
4.1E-8--4.8E-8
|
MHASM2
|
resistivity
converted from conductivity |
| C17000-TH02 (strip) |
36-42
|
|
3.8E-8--4.5E-8
|
MHASM2
|
resistivity
converted from conductivity |
| C17000-TH04 (strip) |
38-45
|
|
4.7E-8--5.2E-8
|
MHASM2
|
resistivity
converted from conductivity |
| C17000-TH04 (rod, bar, plate tubing) |
22-25
|
|
6.9E-8--7.8E-8
|
MHASM2
|
resistivity
converted from conductivity |
| C17000-TM00 (strip) |
33-37
|
|
4.5E-8--5.1E-8
|
MHASM2
|
resistivity
converted from conductivity |
| C17000-TM01 (strip) |
34-38
|
|
4.4E-8--4.9E-8
|
MHASM2
|
resistivity
converted from conductivity |
| C17000-TM02 (strip) |
35-39
|
|
4.3E-8--4.8E-8
|
MHASM2
|
resistivity
converted from conductivity |
| C17000-TM04 (strip) |
36-40
|
|
4.1E-8--4.7E-8
|
MHASM2
|
resistivity
converted from conductivity |
| C17000-TM06 (strip) |
37-42
|
|
4.1E-8--4.7E-8
|
MHASM2
|
resistivity
converted from conductivity |
| C17000-TM08 (strip) |
33-45
|
|
3.8E-8--5.2E-8
|
MHASM2
|
resistivity
converted from conductivity |
| C17000 as-cast (billet) |
16-22
|
|
7.8E-8--1.1E-7
|
MHASM2
|
resistivity
converted from conductivity |
| C17000 cast and aged (billet) |
18-23
|
|
7.5E-8--9.6E-8
|
MHASM2
|
resistivity
converted from conductivity |
| C17200, C17300-TB00 |
17-19
|
|
9.1E-8--1.0E-7
|
MHASM2
|
resistivity
converted from conductivity |
| C17200, C17300-TB00 (billets) |
25-45
|
|
3.8E-8--6.9E-8
|
MHASM2
|
resistivity
converted from conductivity |
| C17200, C17300-TD01 |
16-18
|
|
9.6E-8--1.1E-7
|
MHASM2
|
resistivity
converted from conductivity |
| C17200, C17300-TD02 |
15-17
|
|
1.0E-7--1.1E-7
|
MHASM2
|
resistivity
converted from conductivity |
| C17200, C17300-TD04 |
15-17
|
|
1.0E-7--1.1E-7
|
MHASM2
|
resistivity
converted from conductivity |
| C17200, C17300-TF00 |
22-25
|
|
6.9E-8--7.8E-8
|
MHASM2
|
resistivity
converted from conductivity |
| C17200, C17300-TF00 (billets) |
1.0-3.0
|
|
5.7E-7--1.7E-6
|
MHASM2
|
resistivity
converted from conductivity |
| C17200, C17300-TH01 |
22-25
|
|
6.9E-8--7.8E-8
|
MHASM2
|
resistivity
converted from conductivity |
| C17200, C17300-TH02 |
22-25
|
|
6.9E-8--7.8E-8
|
MHASM2
|
resistivity
converted from conductivity |
| C17200, C17300-TH04 |
22-25
|
|
6.9E-8--7.8E-8
|
MHASM2
|
resistivity
converted from conductivity |
| C17200, C17300-TM00 |
20-28
|
|
6.2E-8--8.6E-8
|
MHASM2
|
resistivity
converted from conductivity |
| C17200, C17300-TM01 |
20-28
|
|
6.2E-8--8.6E-9
|
MHASM2
|
resistivity
converted from conductivity |
| C17200, C17300-TM02 |
20-28
|
|
6.2E-8--8.6E-10
|
MHASM2
|
resistivity
converted from conductivity |
| C17200, C17300-TM04 |
20-28
|
|
6.2E-8--8.6E-11
|
MHASM2
|
resistivity
converted from conductivity |
| C17200, C17300-TM06 |
20-28
|
|
6.2E-8--8.6E-12
|
MHASM2
|
resistivity
converted from conductivity |
| C17200, C17300-TM08 |
20-28
|
|
6.2E-8--8.6E-13
|
MHASM2
|
resistivity
converted from conductivity |
| C17200, C17300 as-cast (billet) |
15-30
|
|
5.7E-8--1.1E-7
|
MHASM2
|
resistivity
converted from conductivity |
| C17200, C17300 cast and aged (billet) |
10.0-20
|
|
8.6E-8--1.7E-7
|
MHASM2
|
resistivity
converted from conductivity |
| C17410 |
45.00
|
|
3.800E-08
|
MHASM2
|
|
| C17500-TB00 |
20-30
|
|
5.7E-8--8.6E-8
|
MHASM2
|
resistivity
converted from conductivity |
| C17500-H04 |
20-30
|
|
5.7E-8--8.6E-9
|
MHASM2
|
resistivity
converted from conductivity |
| C17500-TF00 |
45-60
|
|
2.9E-8--3.8E-8
|
MHASM2
|
resistivity
converted from conductivity |
| C17500-TH04 |
50-60
|
|
2.9E-8--3.4E-8
|
MHASM2
|
resistivity
converted from conductivity |
| C17500-HTR |
45-60
|
|
2.9E-8--3.8E-8
|
MHASM2
|
resistivity
converted from conductivity |
| C17500-HTC |
60 min
|
|
2.9E-8 max
|
MHASM2
|
resistivity
converted from conductivity |
| C17600-TB00 |
20-30
|
|
5.7E-8--8.6E-9
|
MHASM2
|
resistivity
converted from conductivity |
| C17600-TB00 (billet) |
22-28
|
|
6.2E-8--7.8E-8
|
MHASM2
|
resistivity
converted from conductivity |
| C17600-H04 |
20-30
|
|
5.7E-8--8.6E-9
|
MHASM2
|
resistivity
converted from conductivity |
| C17600-TF00 |
45-60
|
|
2.9E-8--3.8E-8
|
MHASM2
|
resistivity
converted from conductivity |
| C17600-TF00 (billet, forged products) |
50-60
|
|
2.9E-8--3.4E-8
|
MHASM2
|
resistivity
converted from conductivity |
| C17600-TH04 |
50-60
|
|
2.9E-8--3.4E-8
|
MHASM2
|
resistivity
converted from conductivity |
| C17600 as-cast (billet) |
32-37
|
|
4.7E-8--5.4E-8
|
MHASM2
|
resistivity
converted from conductivity |
| C17600 cast and aged (billet) |
40-50
|
|
3.4E-8--4.3E-8
|
MHASM2
|
resistivity
converted from conductivity |
| C18100 (annealed) |
80.00
|
|
2.170E-08
|
MHASM2
|
|
| C18200, C18400, C18500-TB00 |
40.00
|
|
4.310E-08
|
MHASM2
|
resistivity
converted from conductivity |
| C18200, C18400, C18500-TH04 |
80.00
|
|
2.163E-08
|
MHASM2
|
|
| C18700 |
96.00
|
|
7.790E-08
|
MHASM2
|
|
| C19200 (strip) |
60.00
|
|
2.880E-08
|
MHASM2
|
|
| C19200 (tubing) |
50.00
|
|
3.450E-08
|
MHASM2
|
|
| C19210 |
80.00
|
|
2.160E-08
|
MHASM2
|
|
| C19400-O60 |
40.00
|
|
4.310E-08
|
MHASM2
|
|
| C19400-H14 |
50.00
|
|
3.450E-08
|
MHASM2
|
|
| C19400 (all other tempers) |
65 nominal
|
|
2.26e-8 nominal
|
MHASM2
|
|
| C19500 |
50.00
|
|
3.440E-08
|
MHASM2
|
|
| C19520 |
40.00
|
|
4.930E-08
|
MHASM2
|
|
| C19700 |
80.00
|
|
2.160E-08
|
MHASM2
|
|
| C21000 (annealed) |
56.00
|
|
3.100E-08
|
MHASM2
|
|
| C22000 (annealed) |
44.00
|
|
3.910E-08
|
MHASM2
|
|
| C22600 (annealed) |
40.00
|
|
4.300E-08
|
MHASM2
|
|
| C23000 (annealed) |
37.00
|
|
4.700E-08
|
MHASM2
|
|
| C24000-O61 |
32.00
|
|
5.400E-08
|
MHASM2
|
|
| C26000-O61 |
28.00
|
|
6.200E-08
|
MHASM2
|
|
| C26800, C27000 (annealed) |
27.00
|
|
6.400E-08
|
MHASM2
|
|
| C28000 |
28.00
|
|
6.160E-08
|
MHASM2
|
|
| C31400 |
42.00
|
|
4.100E-08
|
MHASM2
|
|
| C31600 |
32.00
|
|
5.400E-08
|
MHASM2
|
|
| C33000 |
26.00
|
|
6.600E-08
|
MHASM2
|
|
| C33200-O61 |
26.00
|
|
6.600E-08
|
MHASM2
|
|
| C33500 |
26.00
|
|
6.600E-08
|
MHASM2
|
|
| C34000-O61 |
26.00
|
|
6.600E-08
|
MHASM2
|
|
| C34200, C35300-O61 |
26.00
|
|
6.600E-08
|
MHASM2
|
|
| C34900 |
26.00
|
|
6.600E-08
|
MHASM2
|
|
| C35000 |
26.00
|
|
6.600E-08
|
MHASM2
|
|
| C35600-O61 |
26.00
|
|
6.600E-08
|
MHASM2
|
|
| C36000-O61 |
26.00
|
|
6.600E-08
|
MHASM2
|
|
| C36500, C36600, C36700, C36800-O61 |
28.00
|
|
6.200E-08
|
MHASM2
|
|
| C37000-O61 |
27.00
|
|
6.390E-08
|
MHASM2
|
|
| C37700 |
27.00
|
|
6.400E-08
|
MHASM2
|
|
| C38500-O61 |
28.00
|
|
6.200E-08
|
MHASM2
|
|
| C40500 |
41.00
|
|
4.200E-08
|
MHASM2
|
|
| C40800 |
37.00
|
|
4.660E-08
|
MHASM2
|
|
| C41100 |
32.00
|
|
5.400E-08
|
MHASM2
|
|
| C41500 |
28.00
|
|
6.200E-08
|
MHASM2
|
|
| C41900 |
22.00
|
|
7.800E-08
|
MHASM2
|
|
| C42200 |
31.00
|
|
5.500E-08
|
MHASM2
|
|
| C42500 |
28.00
|
|
6.200E-08
|
MHASM2
|
|
| C43000 |
27.00
|
|
6.400E-08
|
MHASM2
|
|
| C43400 |
31.00
|
|
5.600E-08
|
MHASM2
|
|
| C43500 |
28.00
|
|
6.200E-08
|
MHASM2
|
|
| C44300, C44400, C44500 |
25.00
|
|
6.900E-08
|
MHASM2
|
|
| C46400, C45600, C46600, C46700 (annealed) |
26.00
|
|
6.630E-08
|
MHASM2
|
|
| C48200 |
26.00
|
|
6.630E-08
|
MHASM2
|
|
| C48500 |
26.00
|
|
6.630E-08
|
MHASM2
|
|
| C50500 |
48.00
|