| Material |
Conductivity
|
Resistivity
|
Reference
|
Notes |
|
(% IACS)
|
(Siemens/m)
|
(Ohm-m)
|
(See Below)
|
|
| Magnesium
Alloys (Wrought) |
|
|
|
|
|
| AZ10A |
26.94
|
|
6.400E-08
|
MHASM2
|
conductivity
converted from resistivity |
| AZ31B, AZ31C |
18.50
|
|
9.200E-08
|
MHASM2
|
|
| AZ61A |
11.60
|
|
1.250E-07
|
MHASM2
|
|
| AZ80A |
10.60
|
|
1.450E-07
|
MHASM2
|
|
| HK31A-H24 |
28.26
|
|
6.100E-08
|
MHASM2
|
conductivity
converted from resistivity |
| HK31A-O |
28.74
|
|
6.000E-08
|
MHASM2
|
conductivity
converted from resistivity |
| HM21A-H24 |
33.16
|
|
5.200E-08
|
MHASM2
|
conductivity
converted from resistivity |
| HM21A-O |
34.48
|
|
5.000E-08
|
MHASM2
|
conductivity
converted from resistivity |
| HM31A-F |
26.00
|
|
6.600E-08
|
MHASM2
|
|
| M1A |
34.50
|
|
5.000E-08
|
MHASM2
|
|
| ZC71 |
31.93
|
|
5.400E-08
|
MHASM2
|
conductivity
converted from resistivity |
| ZK60A-F |
29.00
|
|
5.945E-08
|
MHASM2
|
resistivity
converted from conductivity |
| ZK60A-T5 |
30.00
|
|
5.747E-08
|
MHASM2
|
resistivity
converted from conductivity |
| |
|
|
|
|
|
| Magnesium Alloys (Cast) |
|
|
|
|
|
| Pure |
38.60
|
2.239E+07
|
4.467E-08
|
CSNDT
|
|
| Magnesium Alloys (Cast) |
15.00
|
8.700E+06
|
1.149E-07
|
CSNDT
|
|
| AZ80BTA |
10.80
|
6.264E+06
|
1.596E-07
|
CSNDT
|
|
| Magnesium Cast Alloys |
9.00
|
5.220E+06
|
1.916E-07
|
CSNDT
|
|
| A2 80 |
14.60
|
8.468E+06
|
1.181E-07
|
CSNDT
|
|
| A231 |
17.20
|
9.976E+06
|
1.002E-07
|
CSNDT
|
|
| A251 |
12.80
|
7.424E+06
|
1.347E-07
|
CSNDT
|
|
| A261 |
12.30
|
7.134E+06
|
1.402E-07
|
CSNDT
|
|
| T454 |
12.50
|
7.250E+06
|
1.379E-07
|
CSNDT
|
|
| AM100A-F |
11.50
|
|
1.500E-07
|
MHASM2
|
|
| AM100A-T4 |
9.90
|
|
1.750E-07
|
MHASM2
|
|
| AM110A-T6 |
12.30
|
|
1.400E-07
|
MHASM2
|
|
| AZ63A-F |
15.00
|
|
1.150E-07
|
MHASM2
|
|
| AZ63A-T4 |
12.30
|
|
1.400E-07
|
MHASM2
|
|
| AZ63A-T5 |
13.80
|
|
1.250E-07
|
MHASM2
|
|
| AZ81A |
12.00
|
|
1.300E-08
|
MHASM2
|
|
| AZ91A-F |
10.10
|
|
1.700E-07
|
MHASM2
|
|
| AZ91C-F, AZ91E-F |
11.50
|
|
1.500E-07
|
MHASM2
|
|
| AZ91C-T4, AZ91E-T4 |
9.90
|
|
1.750E-07
|
MHASM2
|
|
| AZ91C-T6, AZ91E-T6 |
11.20
|
|
1.515E-07
|
MHASM2
|
|
| AZ92A-F |
12.30
|
|
1.400E-07
|
MHASM2
|
|
| AZ92A-T4 |
10.50
|
|
1.650E-07
|
MHASM2
|
|
| AZ92A-T6 |
12.30
|
|
1.400E-07
|
MHASM2
|
|
| EQ21 |
25.20
|
|
6.850E-08
|
MHASM2
|
|
| EZ33A |
25.00
|
|
7.000E-08
|
MHASM2
|
|
| HK31A-T6 |
22.00
|
|
7.700E-08
|
MHASM2
|
|
| HK31A-H24 |
28.26
|
|
6.100E-08
|
MHASM2
|
conductivity
converted from resistivity |
| HK31A-O |
28.74
|
|
6.000E-08
|
MHASM2
|
conductivity
converted from resistivity |
| HZ32A |
26.50
|
|
9.500E-08
|
MHASM2
|
|
| K1A |
30.25
|
|
5.700E-08
|
MHASM2
|
conductivity
converted from resistivity |
| QE22A |
25.20
|
|
6.850E-08
|
MHASM2
|
|
| QH21A |
25.17
|
|
6.850E-08
|
MHASM2
|
conductivity
converted from resistivity |
| WE43 |
11.65
|
6.800E+06
|
1.480E-07
|
MHASM2
|
conductivity
(IACS) converted from resistivity |
| WE54 |
9.97
|
5.800E+06
|
1.730E-07
|
MHASM2
|
conductivity
(IACS) converted from resistivity |
| ZC63 |
31.93
|
|
5.400E-08
|
MHASM2
|
conductivity
converted from resistivity |
| ZE41A-T5 |
28.74
|
|
6.000E-08
|
MHASM2
|
conductivity
converted from resistivity |
| ZE63A |
30.90
|
|
5.600E-08
|
MHASM2
|
|
| ZH62A |
26.50
|
|
6.500E-08
|
MHASM2
|
|
| ZK51A |
28.00
|
|
6.200E-08
|
MHASM2
|
|
|
|
|
|
|
|
CSNDT=CSNDT
compiled by Eddy Current Technology Incorporated
MHASM2=ASM Metals Handbook--Volume 2, Tenth Edition
Compiled by
the Collaboration for NDT Education.