| Material |
Conductivity |
Resistivity |
Reference |
Notes |
|
(%
IACS) |
(Siemens/m) |
(Ohm-m) |
(See Below) |
|
| Titanium |
|
|
|
|
|
| Titanium |
3.10 |
1.798E+06 |
5.562E-07 |
ECTM |
|
| Titanium |
2.20 |
1.276E+06 |
7.837E-07 |
CSNDT |
|
| ASTM grades 1, 2, 3, 4, 7, and 11 |
3.3-4.1 |
|
4.2E-7--5.2E-7 |
MHASM2 |
conductivity
converted from resistivity |
| Ti-5Al-2.5Sn |
1.10 |
|
1.570E-06 |
MHASM2 |
conductivity
converted from resistivity |
| Ti-5Al-2.5Sn (low O2) |
0.96 |
|
1.800E-06 |
MHASM2 |
conductivity
converted from resistivity |
| Ti-8Al-1Mo-1V |
0.87 |
|
1.990E-06 |
MHASM2 |
conductivity
converted from resistivity |
| Ti-11Sn-1Mo2.25Al-5.0Zr-1Mo-0.2Si |
1.06 |
|
1.620E-06 |
MHASM2 |
conductivity
converted from resistivity |
| Ti-6Al-2Sn-4Zr-2Mo |
0.91 |
|
1.900E-06 |
MHASM2 |
conductivity
converted from resistivity |
| IMI 685 |
1.03 |
|
1.680E-06 |
MHASM2 |
conductivity
converted from resistivity |
| Ti-8Mn |
1.87 |
|
9.200E-07 |
MHASM2 |
conductivity
converted from resistivity |
| Ti-6Al-4V |
1.01 |
|
1.710E-06 |
MHASM2 |
conductivity
converted from resistivity |
| Ti-6AL-4V |
1.00 |
5.800E+05 |
1.724E-06 |
ECTM |
|
| Ti-6Al-6V-2Sn |
1.10 |
|
1.570E-06 |
MHASM2 |
conductivity
converted from resistivity |
| Ti-7Al-4Mo |
1.01 |
|
1.700E-06 |
MHASM2 |
conductivity
converted from resistivity |
| IMI 550 |
1.09 |
|
1.580E-06 |
MHASM2 |
conductivity
converted from resistivity |
| Ti-11.5Mo-Zr-4.5Sn |
1.11 |
|
1.560E-06 |
MHASM2 |
conductivity
converted from resistivity |
| Ti-15V-3Cr-3Al-3Sn |
1.17 |
|
1.470E-06 |
MHASM2 |
conductivity
converted from resistivity |
|
|
|
|
|
|
CSNDT=CSNDT compiled by Eddy Current Technology Incorporated
ECTM=Eddy Current Testing Manual on Eddy Current Method compiled
by Eddy Current Technology Incorporated
MHASM2=ASM Metals
Handbook--Volume 2, Tenth Edition
Compiled by the Collaboration for NDT Education