Accoustic
Properties for
Metals in Liquid Form-
|
Liquid Metals
|
Longitudinal Velocity
|
Density
g/cm3
|
Acoustic Impedance
g/cm2-sec
x105 |
|
cm/µs
|
in/µs
|
|
NaK (69.4% Na) 100° C
|
.231
|
.0909
|
.893
|
2.06
|
|
NaK (69.4% Na) 200° C
|
.225
|
.0886
|
.871
|
1.96
|
|
NaK (69.4% Na) 300° C
|
.220
|
.0866
|
.848
|
1.87
|
|
NaK (69.4% Na) 400° C
|
.215
|
.0846
|
.825
|
1.77
|
|
NaK (69.4% Na) 500° C
|
.210
|
.0827
|
.801
|
1.68
|
|
NaK (69.4% Na) 600° C
|
.205
|
.0807
|
.778
|
1.59
|
|
NaK (69.4% Na) 700° C
|
.200
|
.0787
|
.754
|
1.51
|
|
NaK (69.4% Na) 800° C
|
.195
|
.0768
|
.730
|
1.42
|
|
|
|
|
|
|
|
NaK (53.1% Na) 100° C
|
.219
|
.0862
|
.876
|
1.92
|
|
NaK (53.1% Na) 200° C
|
.214
|
.0843
|
.853
|
1.83
|
|
NaK (53.1% Na) 300° C
|
.209
|
.0823
|
.830
|
1.73
|
|
NaK (53.1% Na) 400° C
|
.204
|
.0803
|
.807
|
1.65
|
|
NaK (53.1% Na) 500° C
|
.199
|
.0783
|
.784
|
1.56
|
|
NaK (53.1% Na) 600° C
|
.199
|
.0783
|
.761
|
1.51
|
|
NaK (53.1% Na) 700° C
|
.189
|
.0744
|
.738
|
1.39
|
|
NaK (53.1% Na) 800° C
|
.184
|
.0724
|
.714
|
1.31
|
|
|
|
|
|
|
|
NaK (28.5% Na) 100° C
|
.204
|
.0803
|
.849
|
1.73
|
|
NaK (28.5% Na) 200° C
|
.198
|
.078
|
.826
|
1.64
|
|
NaK (28.5% Na) 300° C
|
.193
|
.076
|
.804
|
1.55
|
|
NaK (28.5% Na) 400° C
|
.188
|
.074
|
.781
|
1.47
|
|
NaK (28.5% Na) 500° C
|
.182
|
.0717
|
.759
|
1.38
|
|
NaK (28.5% Na) 600° C
|
.177
|
.0697
|
.736
|
1.3
|
|
NaK (28.5% Na) 700° C
|
.172
|
.0677
|
.713
|
1.23
|
|
NaK (28.5% Na) 800° C
|
.166
|
.0654
|
.640
|
1.06
|
|
|
|
|
|
|
|
Potassium 100° C
|
.186
|
.0732
|
.818
|
1.52
|
|
Potassium 200° C
|
.181
|
.0713
|
.796
|
1.44
|
|
Potassium 300° C
|
.176
|
.0693
|
.773
|
1.36
|
|
Potassium 400° C
|
.171
|
.0673
|
.751
|
1.28
|
|
Potassium 500° C
|
.165
|
.065
|
.729
|
1.2
|
|
Potassium 600° C
|
.160
|
.063
|
.707
|
1.13
|
|
Potassium 700° C
|
.155
|
.061
|
.685
|
1.06
|
|
Potassium 800° C
|
.149
|
.0587
|
.662
|
.99
|
|
|
|
|
|
|
|
Sodium 100° C
|
.253
|
.0996
|
.926
|
2.34
|
|
Sodium 200° C
|
.248
|
.0976
|
.904
|
2.24
|
|
Sodium 300° C
|
.242
|
.0953
|
.881
|
2.13
|
|
Sodium 400° C
|
.237
|
.0933
|
.857
|
2.03
|
|
Sodium 500° C
|
.231
|
.0909
|
.883
|
2.04
|
|
Sodium 600° C
|
.226
|
.089
|
.809
|
1.83
|
|
Sodium 700° C
|
.221
|
.087
|
.784
|
1.73
|
|
Sodium 800° C
|
.215
|
.0846
|
.759
|
1.63
|
Data compiled by Xactex Corporation. Sources of original data are unknown.-