Home - General Resources - Material Properties Tables - UT

 

Accoustic Properties for
Metals in Solid Form

 

Metals

Longitudinal Velocity

Shear
Velocity

Surface
Velocity

Density

g/cm3

Acoustic Impedance

g/cm2-sec x
105

cm/µs

in/µs

cm/µs

in/µs

cm/µs

in/µs

Aluminum

0.632

0.2488

0.313

0.1232

N/A
N/A

2.70

17.10

AL 1100-0 (2SO)

0.635

0.25

0.310

0.122

0.290

0.114

2.71

17.20

AL 2014 (14S)

0.632

0.2488

0.307

0.1209

N/A
N/A

2.80

17.80

AL 2024 T4 (24ST)

0.637

0.2508

0.316

0.1244

0.295

0.116

2.77

17.60

AL 2117 T4 (17ST)

0.650

0.2559

0.312

0.1228

N/A
N/A

2.80

18.20

 

 

 

 

 

Babbitt
Bearing

0.230

0.0906

N/A
N/A
N/A
N/A

7.4 -11.0

23.20

Beryllium

1.29

0.5079

0.888

0.3496

0.787

0.310

1.82

23.50

Bismuth

0.218

0.0858

0.110

0.0433

N/A
N/A

9.80

21.40

Brass

0.428

0.1685

0.230

0.0906

N/A
N/A

8.56

36.70

Brass, Half Hard

0.383

0.1508

0.205

0.0807

N/A
N/A

8.10

31.02

Brass, Naval

0.443

0.1744

0.212

0.0835

0.195

0.0770

8.42

37.3

Bronze, Phospho

0.353

0.139

0.223

0.0878

0.201

0.0790

8.86

31.28

 

Cadmium

0.278

0.1094

0.150

0.0591

N/A
N/A

8.64

24.02

Cesium (28.5° C)

0.0967

0.0381

N/A
N/A
N/A
N/A

1.88

1.82

Columbium

0.492

0.1937

0.210

0.0827

N/A
N/A

8.57

42.16

Constantan

0.524

0.2063

0.104

0.0409

N/A
N/A

8.88

46.53

Copper

0.466

0.1835

0.233

0.0890

0.193

0.0760

8.93

41.61

 

Gallium

0.274

0.1079

N/A
N/A
N/A
N/A

5.95

16.3

Germanium

0.541

0.213

N/A
N/A
N/A
N/A

5.47

29.59

Gold

0.324

0.1276

0.120

0.0472

N/A
N/A

19.32

62.6

Hafnium

0.384

0.1512

N/A
N/A
N/A
N/A
N/A
N/A

Inconel

0.572

0.2252

N/A
N/A

0.279

0.110

8.25

47.19

Indium
(156
° C)

0.222

0.0874

N/A
N/A
N/A
N/A

7.30

16.21

Iron

0.590

0.2323

0.323

0.1272

0.279

0.110

7.70

45.43

Iron, Cast

0.480

0.189

0.240

0.0945

N/A
N/A

7.80

37.44

 

 

 

Lead

0.216

0.085

0.070

0.0276

0.0630

0.0248

11.4

24.62

Lead 5% Antinomy

0.217

0.0854

0.081

0.0319

0.0740

0.0291

1.9

23.65

Magnesium

0.631

0.2484

N/A
N/A
N/A
N/A

1.74

10.98

Magnesium (AM-35)

0.579

0.228

0.310

0.122

0.287

0.113

1.74

10.07

Magnesium (FS-1)

0.547

0.2154

0.303

0.1193

N/A
N/A

1.69

9.24

Magnesium (J-1)

0.567

0.2232

0.301

0.1185

N/A
N/A

1.70

9.64

Magnesium (M)

0.576

0.2268

0.309

0.1217

N/A
N/A

1.75

10.08

Magnesium (O-1)

0.580

0.2283

0.304

0.1197

N/A
N/A

1.82

10.56

Magnesium (ZK-60A-TS)

0.571

0.2248

0.305

0.1201

N/A
N/A

1.83

10.45

Manganese

0.466

0.1835

0.235

0.0925

N/A
N/A

7.39

34.44

Molybdenum

0.629

0.2476

0.335

0.1319

0.311

0.122

10.2

64.16

Monel

0.602

0.237

0.272

0.1071

0.196

0.0772

8.83

53.16

 
 
 
 
 

 

 

 

Nickel

0.563

0.2217

0.296

0.1165

0.264

0.104

8.88

49.99

Platinum

0.396

0.1559

0 .167

N/A
N/A
N/A

21.4

84.74

Plutonium

0.179

0.0705

N/A

N/A
N/A
N/A
N/A

28.2

Plutonium (1% Gallium)

0.182

0.0717

N/A
N/A
N/A
N/A
N/A

28.6

Potassium (100° C)

0.182

0.0717

N/A
N/A
N/A
N/A

0.83

1.51

Radium

0.0822

0.0324

0.111

0.0437

0.103

0.0404

5.0

4.11

Rubidium

0.126

0.0496

N/A
N/A
N/A
N/A

1.53

1.93

Silver

0.360

0.1417

0.159

0.0626

N/A
N/A

10.5

37.8

Silver, Nickel

0.462

0.1819

0.232

0.0913

0.169

0.0665

8.75

40.43

Silver, German

0.476

0.1874

N/A
N/A
N/A
N/A

8.70

41.41

Steel, 302 Cres

0.566

0.2228

0.312

0.1228

0.312

0.123

8.03

45.45

Steel, 347 Cres

0.574

0.226

0.309

0.1217

N/A
N/A

7.91

45.4

Steel, 410 Cres

0.539

0.212

0.299

0.118

0.216

0.085

7.67

56.68

Steel, 1020

0.589

0.2319

0.324

0.1276

N/A
N/A

7.71

45.41

Steel, 1095

0.590

0.2323

0.319

0.1256

N/A

N/A

7.80

46.02

Steel, 4150, Rc14

0.586

0.2307

0.279

0.1098

N/A

N/A

7.84

45.94

Steel, 4150, Rc18

0.589

0.2319

0.318

0.1252

N/A
N/A

7.82

46.06

Steel, 4150, Rc43

0.587

0.2311

0.320

0.126

N/A
N/A

7.81

45.84

Steel, 4150, Rc64

0.582

0.2291

0.277

0.1091

N/A
N/A

7.80

45.4

 

 

 

Steel, 4340

0.585

0.2303

0.128

0.0504

N/A
N/A

7.80

45.63

Tantalum

0.410

0.1614

0.114

0.0449

N/A
N/A

16.6

68.06

Thallium (302° C)

0.162

0.0638

N/A
N/A
N/A
N/A

11.9

19.28

Thorium

0.240

0.0945

0.156

0.0614

N/A
N/A

11.3

27.12

Tin

0.332

0.1307

0.167

0.0657

N/A
N/A

7.29

24.2

Titanium

0.607

0.239

0.331

0.1303

N/A
N/A

4.50

27.32

 

 

 

 

Titanium Carbide

0.827

0.3256

0.516

0.2031

N/A
N/A

5.15

42.59

Tungsten

0.518

0.2039

0.287

0.113

0.265

0.104

19.25

99.72

Uranium

0.338

0.1331

0.196

0.0772

N/A
N/A

18.9

63.88

Uranium Dioxide

0.518

0.2039

N/A
N/A
N/A
N/A

6.03

31.24

Vanadium

0.600

0.2362

0.278

0.1094

N/A
N/A

6.03

36.18

Zinc

0.417

0.1642

0.241

0.0948

N/A
N/A

7.10

29.61

Zircaloy

0.472

0.1858

0.236

0.093

N/A
N/A

9.03

42.6

Zirconium

0.465

0.1831

0.222

0.0874

N/A
N/A

6.48

30.1

Data compiled by Xactex Corporation.  Sources of original data are unknown.-