Home - General Resources - Material Properties Tables - UT
Plastics, Resins, and Phenolics
Longitudinal Velocity
Shear Velocity
Density
g/cm3
Acoustic Impedance
g/cm2-sec x105
cm/µs
in/µs
Acrylic Resin
.267
.1051
.112
.0441
1.18
3.151
Bakelite
.259
.102
N/A
1.40
3.626
Bakelite (cloth filled)
.271
.1067
Cellulose Acetate
.245
.0965
1.30
3.185
Hysol
.277
.1091
Kel-F
.179
.0705
Lucite
.268
.1055
.126
.0496
3.1624
Micarta Linen base
.3
.1181
Nylon 6,6
.168
.0661
Nylon
.262
.1031
Phenolic
.142
.0559
1.34
1.903
Plexiglass (a) UVA
.276
.1087
1.27
3.505
(b) UVAII
.273
.1075
.143
.0563
3.221
Polyethylene
1.10
2.937
Polyethylene TCI
.16
.063
Polyimide (Vespel SP-1)
.244
.0961
1.48
3.61
Polystyrene
Polystyrol
.15
.0591
Refrasil
.375
.1476
1.73
6.488
Teflon
.135
.0531
2.20
2.97
Data compiled by Xactex Corporation. Sources of original data are unknown.
-