Home - General Resources - Material Properties Tables - UT
Powered Metal and Materials
Longitudinal Velocity
Shear Velocity
Surface Velocity
Density g/cm3
Acoustic Impedance g/cm2-sec x105
cm/µs
in/µs
Rene (Cabot)
R-41 (53NI-19Cr-11Co-10Mo)
.604
.2378
.32
.126
.297
.117
6.25
49.8
R-77 (55NI-15Co-15Cr)
.62
.2441
.329
.1295
.305
.12
7.92
49.1
R-80 (6.5NI-9.9Co-14Cr)
.594
.2339
.323
.1272
N/A
R-95 (6lNf-8Co-14Cr)
.597
.235
8.19
48.9
-60 Mesh
.589
.2319
8.08
47.6
-As-HIP'd
.605
.2382
.302
.1189
-Cast & Wrought
.294
.1157
- HIP'D & Forged
-150 Mesh
.603
.2374
8.30
50.0
-As HIP'd
.613
.2413
Wrought
.607
.239
.321
.1264
.298
8.22
49.9